Home \ Browse Journal \ 2025 \ 2025 Volume 8 Issues 1–3 \ Synthesis of Polysiloxane–(Butylene Oxide)–Urethane–Ureas in the Presence of Bismuth(III) Neodecanoate

2025 Volume 8 Issues 1–3

инэос-open
Open Access
cc-by-nc

INEOS OPEN, 2025, 8 (1–3), 106–107

Journal of Nesmeyanov Institute of Organoelement Compounds
of the Russian Academy of Sciences

Download PDF
Electronic supplementary information
DOI: 10.32931/io2539a

issue_cover_8_1-3.png       

Synthesis of Polysiloxane–(Butylene Oxide)–Urethane–Ureas
in the Presence of Bismuth(III) Neodecanoate

L. V. Filimonova,*a M. I. Buzin,a G. G. Nikiforova,a I. O. Volkov,a E. S. Afanasyev,a K. L. Boldyrev,a
D. A. Khanin,a Z. S. Klemenkova,a R. U. Takazova,a E. S. Trankina,a V. S. Papkov,a and A. M. Muzafarova,b

a Nesmeyanov Institute of Organoelement Compounds, Russian Academy of Sciences, ul. Vavilova 28, str. 1, Moscow, 119334 Russia
b Enikolopov Institute of Synthetic Polymeric Materials, Russian Academy of Sciences, ul. Profsoyuznaya 70, Moscow, 117393 Russia

 

Corresponding author: L. V. Filimonova, e-mail: lufilia@inbox.ru
Received 10 November 2024; accepted 17 January 2025

Abstract

io2539a_abs_fig

Polysiloxane–(butylene oxide)–urethane–ureas were synthesized in the presence of bismuth(III) neodecanoate. The resulting polymers were studied by differential scanning calorimetry (DSC), thermomechanical analysis (TMA), optical and atomic force microscopy (AFM); their deformation and strength characteristics were determined. It was found that the polymers obtained are characterized by two glass transition temperatures, indicating the formation of two phases.

Key words: polysiloxanes, polyurethanes, microphase separation, catalyst, atomic force microscopy.

 

Introduction

Polysiloxane–urethanes (PSUs) are of great interest since they can combine the unique properties of polysiloxanes (low glass transition temperature, low surface energy, hydrophobicity, high gas permeability, biological inertness) and polyurethanes (high mechanical strength) [1, 2]. Toxic organotin catalysts are widely used in the synthesis of polyurethanes. Bismuth-based catalysts have lower toxicity and can also be used in the synthesis [1, 3, 4].

In this work, cross-linked polysiloxane–(butylene oxide)–urethane ureas (PSBOUUrs) were synthesized based on α,ω-bis[(3-aminopropyl)diethoxy]-oligodimethylsiloxanes (DASs) and oligobutylene oxides (OBOs), 4,4'-dicyclohexylmethane diisocyanate (H12-MDI) or isophorone diisocyanate (IPDI) in the presence of bismuth(III) neodecanoate used as a catalyst, as well as model polybutylene oxide–urethanes and polysiloxane–ureas were obtained by the earlier published method [5], and their properties were studied.

Results and discussion

PSBOUUrs were synthesized according to the general scheme (Scheme 1). At the first stage (I), prepolymer A was obtained from diisocyanate and oligobutylene oxide. The reaction course was monitored by back titration of free isocyanate groups and by IR spectroscopy (see Table S5 and Fig. S2 in the Electronic supplementary information (ESI)). The second stage (II) was carried out by combining solutions of the prepolymer and DAS, which resulted in the formation of soluble PSBOUUr B. At the third stage (III), the evaporation of the solvents resulted in the cleavage of hydrolytically unstable ethoxy groups, followed by the condensation of the resulting SiOH groups and the formation of cross-linked polymer C.

  XHO(R) m H + ( X+1)OCNR'NCO + SiO OEt OEt (CH 2 ) 3 H 2 N SiO Me Me Si OEt OEt (CH 2 ) 3 NH 2 {CNHR'NHC[O (R) m CNHR'NHC] x-1 O(R) m CNHR'NHCNH (CH 2 ) 3 SiO OEt OEt SiO Me Me Si OEt OEt (CH 2 ) 3 NH} p O O O O O O OCNR'NHC[O (R) m CNHR'NHC] x-1 O(R) m CNHR'NCO O O O Cat I II + H 2 O – EtOH III {CNHR'NHC[O (R) m CNHR'NHC] x-1 O(R) m CNHR'NHCNH (CH 2 ) 3 SiO O O SiO Me Me Si O O (CH 2 ) 3 NH} p O O O O O O Si Si A B C R = R' = CH 2 H 12 – MDI X = 1,2 IPDI ( ) n ( ) n ( ) n (CH 2 ) 4 O O

Scheme 1. Synthesis of polysiloxane–(butylene oxide)–urethane–ureas.

The resulting polymers were studied by DSC, TMA, AFM, and optical microscopy. The main properties of PSBOUUrs, as well as those of the model polyurethanes and polysiloxane–ureas are given in Table 1 and Tables S1–S4 in the ESI.

Table 1. Effect of the synthesis conditions on the thermal and mechanical properties of the resulting polysiloxane–(butylene oxide)–urethane–ureas

PSBOUUr
DAS, n/Mn
OBO, m/Mn
DI
Wsil, wt %
Solvent
Gel fraction, %
Тg
εр, %
σр, MPa
1a
14/1380
3/250
Н12-MDI
47
MEK
78
–113/60
82
15
2a
14/1380
3/250
Н12-MDI
47
MEK + hexane
79
–121/52c
160
14
3b
25/2230
18/1060
Н12-MDI
53
MEK + hexane
78
–18/–63
320
2
4b
25/2230
18/1060
IPDI
52
MEK + hexane
88
–118/–76
230
1.5
a X = 2; b X =1; c the glass transition temperature was determined by TMA; Wsil is the total content of the siloxane, including terminal groups after the network formation.

As can be seen from Tables 1 and S4 in the ESI, the introduction of an organic block improves the mechanical properties and significantly increases a relative elongation at break of PSBOUUrs compared to the model polysiloxane–ureas.

All PSBOUUrs obtained had a high content of gel fraction, which characterizes the degree of completion of the cross-linking process. The content of the siloxane component in all samples was ~50%, but PSBOUUr 1 and PSBOUUr 2 had much higher tensile strength, which is probably due to the increased concentration of urethane units and hydrogen bonds in this case. A characteristic feature of PSUs is their tendency to microphase separation caused by the thermodynamic incompatibility of the components, which can be judged, in particular, by the difference in their solubility parameters (oligobutylene oxide: δ = 19.2 (MPa)0.5, oligodimethylsiloxane: δ = 14.6 (MPa)0.5 [6]). For all the resulting PSBOUUrs, two glass transition temperatures were observed, indicating the formation of two-phase systems. Some discrepancy between the values of Tg of PSBOUUrs and model polymers is likely to be due to the effect of several factors, which include the phase mixing and presence of a chemical network.

From the results of atomic force and optical microscopy studies (Figs. 1 and S3 in the ESI, respectively), it is evident that PSBOUUr1 obtained from a solution in methyl ethyl ketone (MEK) exhibits a large relief and aggregates, the sizes of which can reach several microns or more.

io2539a_fig1

Figure. 1. AFM images of PSBOUUrs: 1 (a), 2 (b), 3 (c), 4 (d).

Vshivkov et al. [7] found that polydimethylsiloxane forms associates in MEK. This can promote gelation in solutions and lead to the formation of heterogeneous samples. To prevent gelation, hexane, which is a good solvent for polydimethylsiloxane, was used in the synthesis [8]. The prepolymer was dissolved in MEK, and the oligodiamine was dissolved in hexane. In PSBOUUrs solutions, the ratio of MEK to hexane was 1:1 (v/v). The addition of hexane afforded homogeneous films with microphase separation and led to an increase in the relative elongation at break.

Conclusions

Hence, polysiloxane–(butylene oxide)–urethane–ureas and model polybutylene oxide–urethanes were synthesized in the presence of Bi(III) neodecanoate used as a catalyst. It was shown that the introduction of the oligobutylene oxide block improves the mechanical characteristics compared to the model polysiloxane–urea with the same length of the siloxane moiety. The resulting PSBOUUrs were found to feature two glass transition temperatures, which indicates the formation of two phases. The effect of the solvent on the surface morphology was detected by AFM.

Acknowledgements

This work was supported by the Ministry of Science and Higher Education of the Russian Federation (agreement no. 075-00276-25-00) using the equipment of the Center for Collective Use of INEOS RAS.

The authors are grateful to L. I. Makarova, O. V. Sinitsyna, and I. V. Yaminsky for fruitful discussions.

Electronic supplementary information

Electronic supplementary information (ESI) available online: the experimental section, GPC data for the model polyurethanes, IR spectrum of the prepolymer, optical micrographs. For ESI, see DOI: 10.32931/io2539a.

References

  1. M. F. Sonnenschein, Polyurethanes. Science, Technology, Markets, and Trends, Wiley, Hoboken, 2015. DOI: 10.1002/9781118901274
  2. AU Patent 779389B2, 2000.
  3. D. Guhl, Proc. Eur. Coatings Conf.: Polyurethanes for High Performance Coatings, 2008, 119–137. DOI: 10.13140/2.1.2416.3209
  4. M. S. Shabalina, E. A. Antipova, G. A. Khlebov, Int. Polym. Sci. Technol., 2015, 42, T21–T24. DOI: 10.1177/0307174x1504200605
  5. L. V. Filimonova, G. G. Nikiforova, M. I. Buzin, E. S. Afanasyev, K. L. Boldyrev, Z. S. Klemenkova, R. U. Takazova, E. S. Trankina, D. A. Khanin, A. M. Muzafarov, INEOS OPEN, 2022, 5, 161–164. DOI: 10.32931/io2229a
  6. R. Benrashid, G. L. Nelson. J. Polym. Sci.: Part A: Polym. Chem., 1994, 32, 1847–1865. DOI: 10.1002/pola.1994.080321006.
  7. S. A. Vshivkov, E. V. Rusinova, V. N. Dubchak, G. B. Zarubin, Polym. Sci., Ser. A, 1996, 38, 563–569.
  8. Yu. S. Lipatov, A. E. Nesterov, T. M. Gritsenko, R. A. Veselovskii, Handbook of Polymer Chemistry, Naukova Dumka, Kiev, 1971 (in Russian).